Skip to main content

Official Journal of the Japan Wood Research Society

Table 2 Effect of different heating exposure time on heartwood color under 170 °C

From: Effects of heat treatment on water-soluble extractives and color changes of merbau heartwood

Heat treatment conditions

ΔL *

Δa *

Δb *

ΔE *

Heating temperature (°C)

Heating time elapsed (h)

Control

0.0

0.0

0.00

0.0

170

1

−18.1

6.7

−9.0

21.3

2

−22.5

2.3

−10.6

25.0

3

−23.4

−15.2

−9.4

29.5

4

−32.5

−21.7

−12.6

41.1

5

−31.1

−24.1

−14.1

41.8