Table 2 Surface roughness and Janka hardness values of the samples

From: Surface quality and hardness of eastern redcedar as function of steaming

Sample type

Density (g/cm3)

Roughness parameters (µm)

Janka hardness (kg)

R a

R z

A

0.482

4.65 (0.73)a

44.39 (5.76)

379 (39.60)

B

0.491

5.03 (0.75)

34.49 (6.74)

373 (39.40)

C

0.479

7.06 (0.76)

48.66 (6.68)

399 (34.32)

D

0.471

7.33 (0.80)

49.48 (7.01)

409 (28.59)

E

0.470

7.34 (0.68)

49.24 (7.89)

345 (30.01)

F

0.463

7.43 (0.76)

51.34 (6.79)

355 (29.56)

  1. aNumbers in parentheses are standard deviation values