Table 4 Modulus of rupture (MOR) of particleboard subjected to outdoor exposure at the eight sites

From: Effectiveness of principal component analysis for analyzing particleboard subjected to outdoor exposure

 

MOR (MPa)

Exposure term (year)

1

2

3

4

5

Site 1

14.9 (1.63)

13.7 (1.10)

12.8 (1.87)

11.8 (1.75)

6.34 (1.50)

Site 2

14.9 (1.60)

14.1 (1.87)

9.63 (1.48)

9.41 (3.12)

10.3 (3.22)

Site 3

13.2 (0.91)

11.5 (2.13)

10.6 (1.05)

8.69 (0.83)

4.01 (0.45)

Site 4

14.1 (1.60)

12.5 (1.01)

9.85 (2.15)

7.70 (2.91)

9.44 (2.55)

Site 5

12.9 (1.38)

9.90 (2.48)

7.05 (0.63)

6.28 (1.94)

4.69 (0.94)

Site 6

14.0 (1.48)

8.33 (1.26)

7.65 (1.88)

4.77 (1.40)

5.22 (1.23)

Site 7

11.9 (2.31)

8.90 (1.54)

6.67 (0.73)

5.79 (0.87)

5.07 (1.09)

Site 8

7.90 (1.90)

7.17 (2.43)

5.86 (1.51)

5.14 (0.45)

4.88 (0.73)

  1. Site nos. are listed in Table 1
  2. Numbers in parentheses indicate standard deviations