Table 4 Modulus of rupture (MOR) retention and internal bond strength (IB) retention of boards subjected to various exposure conditions

From: Bending strength and internal bond strength of wood-based boards subjected to various exposure conditions

Exposure condition

MOR retention (%)

IB retention (%)

PF board

MDI board

Aspen board

Pine board

F-MDI board

F-MUF board

PF board

MDI board

Aspen board

Pine board

F-MDI board

F-MUF board

5-year high humidity

67.3

85.0

74.1

81.4

89.6

78.6

83.1

84.5

68.5

81.9

96.3

97.0

5-year cyclic humidity

74.6

94.9

63.8

91.5

90.3

86.5

68.9

86.5

32.8

72.3

91.0

100

1-year outdoor

69.2

84.4

75.8

82.2

89.7

87.6

72.9

84.9

69.5

89.6

93.1

100

3-year outdoor

48.5

68.1

53.3

61.4

79.8

70.9

38.4

84.3

56.6

84.0

81.3

100

5-year outdoor

46.5

70.6

39.1

48.5

77.1

62.0

16.9

67.6

32.8

48.5

96.7

87.8

JIS Test B

59.6

90.9

100

66.0

16.9

66.2

21.4

35.9

86.9

61.3

  1. Abbreviations are explained in Table 1. 5-year high humidity, 5-year exposure to relative humidity of 90 %. 5-year cyclic humidity, 5-year exposure to cycles of relative humidity of 45 % at 20 °C for 3 months and 90 % at 20 °C for 3 months (1 cycle: 6 months; 10 cycles:, 5 years). 1-, 3-, and 5-year outdoor, 1-, 3-, and 5-year outdoor exposure in Tsukuba, Japan, respectively. JIS Test B, accelerated aging test in compliance with Test B in JIS A 5908 [21] or JIS A 5905 [22] (boiling for 2 h and subsequent water soaking for 1 h at room temperature). The retention that exceeds 100 % is recorded as 100 %