Skip to main content

Official Journal of the Japan Wood Research Society

Table 6 Thickness change and mass loss of boards subjected to various exposure conditions

From: Bending strength and internal bond strength of wood-based boards subjected to various exposure conditions

Exposure condition

Thickness change (%)

Mass loss (%)

PF board

MDI board

Aspen board

Pine board

F-MDI board

F-MUF board

PF board

MDI board

Aspen board

Pine board

F-MDI board

F-MUF board

5-year high humidity

3.34

2.65

7.64

6.60

1.66

2.38

0

0

0

0

0

0

5-year cyclic humidity

2.66

2.12

10.8

5.14

1.00

1.32

0

0

0

0

0

0

1-year outdoor

3.16

2.51

10.5

6.37

0.397

1.02

0

0

0

0

0

0

3-year outdoor

6.02

4.08

12.6

8.82

0.746

2.32

1.59

0.67

1.62

0

0

0

5-year outdoor

15.2

4.01

16.0

10.7

−0.130

2.01

4.34

2.54

6.65

2.37

2.37

1.79

JIS Test B

16.7

4.90

21.1

13.5

1.50

9.70

2.40

1.20

1.20

0.70

0.70

1.90

  1. Abbreviations are explained in Table 1. 5-year high humidity, 5-year exposure to relative humidity of 90 %. 5-year cyclic humidity, 5-year exposure to cycles of relative humidity of 45 % at 20 °C for 3 months and 90 % at 20 °C for 3 months (one cycle: 6 months; 10 cycles: 5 years). 1-, 3-, and 5-year outdoor, 1-, 3-, and 5-year outdoor exposure in Tsukuba, Japan, respectively. JIS Test B, accelerated aging test in compliance with Test B in JIS A 5908 [21] or JIS A 5905 [22] (boiling for 2 h and subsequent water soaking for 1 h at room temperature)