Skip to main content

Official Journal of the Japan Wood Research Society

Table 1 Mass-loss rates of 4 wood samples after eight-week decay tests and five wood samples after twelve-week decay tests

From: Wood decaying properties of the termite mushroom Termitomyces eurrhizus

Strains

The mass loss rates of decay samples

P. densiflora

C. japonica

Heartwood

Sapwood

Heartwood

Sapwood

8-week

SD

12-week

SD

8-week

SD

12-week

SD

8-week

SD

12-week

SD

8-week

SD

12-week

SD

T3

6.7

0.4B

8.2

1.5A*

8.7

0.2A

7.3

0.6A

4.7

1.8D

2.2

3.5B*

8.8

2.2CD

1.8

2.2B

T11

6.6

0.7B

7.6

1.2A

7.6

0.1AB

4.8

1.0B

10.1

1.6AB*

1.1

2.8C*

7.5

3.0CD

4.4

1.8B

T25

3.5

0.4C

  

6.0

0.3B

  

4.4

1.3D*

  

5.5

1.5D

  

T26

6.8

0.5B

8.3

0.9A*

8.3

0.4A

7.9

0.7A

5.6

0.7CD

4.9

2.2B

10.8

2.6C

8.4

0.7A

T. versicolor

8.3

0.8B*

8.5

2.9A*

7.0

1.3AB

8.0

2.0A

11.5

1.1A

−5.2

9.7BC*

16.7

0.6B

3.7

2.7B

F. palustris

16.3

2.0A

9.0

1.3A*

5.5

2.0B

8.1

0.8A

8.0

1.4BC

9.4

1.8A*

22.7

0.7A

9.9

1.1A

Strains

The mass loss rates of decay samples

C. obtusa

F. crenata

Heartwood

Sapwood

Heartwood

Sapwood

8-week

SD

12-week

SD

8-week

SD

12-week

SD

8-week

SD

12-week

SD

8-week

SD

12-week

SD

T3

7.8

0.5B

7.0

1.0C*

11.7

0.4BC

7.9

0.9B

2.3

0.2C

4.4

0.3B*

5.3

0.2B

4.2

0.4B

T11

10.2

0.4A*

7.7

0.7BC*

8.7

1.2C

6.4

1.6B

2.3

0.5C

1.4

1.0C*

3.7

0.3B

0.9

1.7C

T25

5.2

1.1C

  

7.2

0.8D

  

0.9

0.5C

  

3.2

0.5B

  

T26

9.4

0.8AB

10.2

0.5A*

12.0

0.8B

10.0

0.6A

2.4

0.4C

4.2

0.3B*

4.7

0.2B

4.8

0.4B

T. versicolor

7.8

1.5B

−7.8

3.9D

14.5

2.2B

6.5

6.8AB

15.3

3.2A*

17.9

5.0A*

17.9

3.6A

26.1

12.3A

F. palustris

5.2

1.1C

8.6

0.4B

21.1

2.2A

10.0

0.5A

8.5

6.6B*

5.2

0.5B

15.2

1.0A

4.5

0.1B

Strains

The mass loss rates of decay samples

Q. miyagii

 

Heartwood

Sapwood

  

8-week

SD

12-week

SD

8-week

SD

12-week

SD

        

T3

  

0.5

0.3B

  

2.1

0.7C

        

T11

  

1.2

0.6AB

  

2.4

0.2C

        

T25

                

T26

  

1.0

0.3A

  

3.0

0.2B

        

T. versicolor

  

1.1

2.4ABC

  

5.1

1.9A

        

F. palustris

  

−0.3

0.2C

  

2.2

0.3C

        
  1. The same characters indicate no significant difference by Tukey–Kramer test (p > 0.05)
  2. The samples for the 8-week test were taken from different logs with samples for 12-week test
  3. The mass-loss rates for 8-week decayed samples cannot be compared with those for 12-week decayed ones
  4. SD standard deviation of mass-loss rate
  5. * There was no significant difference between heartwood and sapwood (t-test p > 0.05)