Skip to main content

Official Journal of the Japan Wood Research Society

Table 1 Chemical analysis of the wood components of untreated and heat-treated eucalypt wood

From: Changes of chemical properties and the water vapour sorption of Eucalyptus pellita wood thermally modified in vacuum

Composition

Untreated

Heat treat temperature (°C)

160

180

200

220

240

Klason lignin* (%)

30.88

32.29

32.39

32.53

33.45

35.30

Holocelllulose* (%)

74.25

68.17

65.68

62.17

56.17

47.06

Alpha-cellulose in holocellulose* (%)

45.42

41.83

40.76

39.02

33.97

23.11

Alcohol-benzene solubility* (%)

1.59

1.93

1.98

2.08

2.79

3.94

1% NaOH solubility* (%)

13.14

18.02

17.72

17.30

16.68

15.76

  1. * Thermo-vacuum treatment was performed for 4 h under the negative pressure (−0.02 to −0.08 MPa)