Official Journal of the Japan Wood Research Society
From: Potential utilization of sodium fluoride (NaF) as a biocide in particleboard production
NaF (%) | Oven-dried density (g/cm3) | MCa (%) | MORb (MPa) | MOEc (MPa) |
---|---|---|---|---|
0.00 | 0.62 | 6.15 (0.31) a | 22.55 (6.34) a | 2499 (522) a |
1.00 | 0.71 | 6.05 (0.19) a | 20.50 (3.64) a | 2318 (301) a |
1.50 | 0.65 | 6.30 (0.13) a | 21.40 (3.85) a | 2419 (355) a |
3.00 | 0.67 | 6.12 (0.16) a | 23.05 (2.58) a | 2551 (253) a |
p values | Â | 0.248 | 0.738 | 0.721 |