Table 4 Retentions of mechanical properties for panels subjected to six different exposure conditions

From: The evaluation of long-term mechanical properties of wood-based panels by indoor exposure tests

Panels

Mild humidity

Semi-mild humidity

High humidity

Cyclic humidity

Roof sheathing

Ceiling of eave

6-y

10-y

5-y

1/4-y

1/2-y

1-y

2-y

3-y

5-y

1/2-y

1-y

3/2-y

2-y

3-y

5-y

9.5-y

9.5-y

Retention of bending strength, MOR (%)

 OSB(A)

87

71 a

75

83

75

76

76

74

81

70

76

74

79

64

100

84

 OSB(P)

91

95

91

100

86

98

83

81

90

77

97

94

96

92

98

97

 PB(P)

96

96

83

100

100

87

72

67

90

85

98

86

88

75

100

100

 PB(I)

100

100

100

99

99

96

92

85

100

100

99

94

100

95

100

100

 MDF(M)

100

100

94

94

95

95

89

79

89

95

98

92

92

87

100

100

 PW(P)

75

75

80

78

79

88

75

80

65

68

100

80

80

88

100

100

Retention of modulus of elasticity, MOE (%)

 OSB(A)

83

69

79

83

64

75

62

62

76

67

77

69

63

56

96

77

 OSB(P)

85

91

86

94

79

88

76

73

88

78

93

84

84

74

100

99

 PB(P)

91

90

85

94

97

80

67

66

90

84

95

81

80

72

100

100

 PB(I)

100

94

100

98

96

92

84

75

100

96

100

89

87

90

100

98

 MDF(M)

100

99

95

94

93

96

85

75

92

92

96

91

85

84

100

100

 PW(P)

85

85

87

80

97

91

80

89

93

85

100

88

78

85

100

86

Retention of internal bond strength, IB (%)

 OSB(A)

61

71

64

68

66

65

70

67

69

62

56

63

55

75

33

86

76

 OSB(P)

83

90

92

88

94

82

93

68

82

100

80

77

75

86

72

88

89

 PB(P)

87

78

90

84

92

83

78

52

83

88

75

79

79

90

69

75

80

 PB(I)

89

86

93

100

95

90

89

85

85

100

100

99

89

93

87

84

88

 MDF(M)

100

100

100

100

100

77

100

100

97

100

100

100

95

100

100

88

100

 PW(P)

93

98

100

79

94

100

100

76

100

100

90

100

84

89

74

77

100

Retention of internal lateral nail resistance, LNR (%)

 OSB(A)

100

94

87

87

87

99

100

100

93

100

100

89

100

100

92

85

88

 OSB(P)

88

98

100

99

100

100

100

100

100

100

100

91

79

100

100

100

100

 PB(P)

94

88

100

100

100

99

96

100

100

100

100

98

100

100

99

76

99

 PB(I)

100

100

100

100

100

100

100

100

99

100

100

100

100

100

100

100

100

 MDF(M)

100

100

100

100

100

100

100

100

99

99

100

99

98

100

99

100

98

 PW(P)

100

100

100

99

100

100

100

100

98

98

90

97

100

100

100

95

94

Retention of nail-head pull-through resistance, NHPT (%)

 OSB(A)

99

97

100

75

77

100

100

89

100

90

81

95

94

96

93

80

81

 OSB(P)

100

95

95

94

97

100

86

95

100

100

100

100

96

100

100

74

88

 PB(P)

100

94

95

94

96

94

88

95

91

72

94

96

98

93

91

84

84

 PB(I)

100

95

100

90

96

99

93

98

92

72

93

96

91

100

96

83

86

 MDF(M)

98

100

99

96

95

99

100

95

99

77

99

99

99

100

99

76

90

 PW(P)

100

100

100

93

100

100

100

88

100

96

95

100

100

100

100

94

97

  1. OSB, PB, MDF, PW see Table 1
  2. aRetentions less than three quarters of the initial values are shown in italic bold, ‘-y’ shows ‘-year’