Table 6 Mean values and standard deviations of lumber properties in each sawing pattern

From: Bending properties of dimension lumber produced from Siberian larch (Larix sibirica) in Mongolia

Lumber type

n

ARW (mm)

AD (g/cm3)

MOE (GPa)

MOR (MPa)

Mean

SD

Mean

SD

Mean

SD

Mean

SD

I

57

2.1a

1.1

0.59a

0.05

9.28a

2.21

43.2a

12.5

II

104

2.0a

1.1

0.60a

0.04

10.15a

2.36

52.3b

21.4

III

29

1.9a

1.2

0.65b

0.04

10.14a

2.92

57.4b

25.2

  1. The same letters (a and b) followed by mean values indicate no significance at the 5% level according to the Tukey–HSD test. The values of the MOE and MOR were adjusted to the values at 15% moisture content
  2. n number of lumber pieces, ARW annual ring width, AD air-dry density at testing, MOE modulus of elasticity, MOR modulus of rupture, SD standard deviation, I lumber including pith at an almost-center position in cross-section, II lumber obtained near the pith (sometimes including pith on the surface area of the lumber), III lumber obtained from outer part of the logs (without pith)