Skip to main content

Official Journal of the Japan Wood Research Society

Table 1 Chemical composition of pulp samples

From: Effects of residual lignin and cellulose swelling on the rate of enzymatic saccharification of softwood and hardwood acid sulfite pulps

 

Yield (%)

Kappa number

Glucan (%)

Xylan (%)

Mannan (%)

Lignin (%)

Acacia SP a

57.3

52.3

70.2

12.8

0

9.9

Acacia SP b

63.3

57.9

58.2

9.6

1.6

10.4

Acacia SPc

53.0

23.0

72.9

6.8

1.1

4.1

Acacia KP

56.0

22.8

67.1

13.0

1.1

3.0

Larch SPd

58.6

74.6

74.9

0

8.7

16.0

Larch SPe

74.8

127

55.8

0.9

16.0

22.8

Larch SPf

57.6

64.3

73.5

3.8

4.8

11.6

Larch soda-AQ

48.0

56.6

44.3

4.6

7.8

7.4

Larch soda-AQ

53.8

25.5

56.8

3.4

6.6

3.8

  1. Cooking conditions
  2. apH 1.4, 145 ℃ for 0.5 h
  3. bpH 2.0, 135 ℃ for 4 h
  4. cpH 2.0, 145 ℃ for 3 h
  5. dpH 1.4, 145 ℃ for 1 h
  6. epH 2.0, 145 ℃ for 1.5 h
  7. fpH 2.0, 145 ℃ for 2 h