Official Journal of the Japan Wood Research Society
From: The effect of oil heat treatment on biological, mechanical and physical properties of bamboo
T/°C | t/h | Oven-dried shrinkage/% | Air-dried shrinkage /% | Weight loss/% | ||||
---|---|---|---|---|---|---|---|---|
Radial | Tangential | Volume | Radial | Tangential | Volume | Â | ||
Untreated |  | 4.22 | 5.42 | 9.68 | 3.74 | 5.30 | 9.68 | – |
140 | 2 | 4.16 | 5.39 | 9.36 | 3.44 | 5.17 | 9.36 | 2.56 |
4 | 4.17 | 5.45 | 11.04 | 3.34 | 4.32 | 7.38 | 3.76 | |
6 | 4.16 | 5.27 | 8.55 | 3.14 | 3.89 | 7.26 | 3.81 | |
160 | 2 | 3.75 | 5.42 | 9.47 | 3.42 | 4.22 | 8.34 | 3.73 |
4 | 4.03 | 5.31 | 9.27 | 3.23 | 4.11 | 6.94 | 3.92 | |
6 | 4.01 | 5.02 | 8.96 | 3.02 | 3.54 | 6.57 | 3.89 | |
180 | 2 | 3.39 | 4.66 | 8.36 | 3.32 | 3.34 | 6.71 | 8.60 |
4 | 3.15 | 4.35 | 7.43 | 2.64 | 3.47 | 6.55 | 8.35 | |
6 | 3.09 | 2.22 | 5.43 | 2.16 | 1.97 | 4.48 | 8.50 | |
200 | 2 | 1.66 | 1.86 | 2.75 | 1.76 | 2.21 | 3.52 | 14.91 |
4 | 1.60 | 1.49 | 4.21 | 1.61 | 2.57 | 5.04 | 18.14 | |
6 | 0.74 | 1.44 | 2.37 | 1.55 | 1.90 | 3.95 | 18.64 |