Official Journal of the Japan Wood Research Society
Specimens | Initial stiffness | Yielding point | Maximum point | Failure point | Ductility ratio | |||
---|---|---|---|---|---|---|---|---|
Ke (kN·m/°) | My (kN·m) | θy (°) | Mp (kN·m) | θp (°) | Mf (kN·m) | θf (°) | μ = θf/θy | |
BC1 | 10.46 | 10.63 | 1.58 | 16.56 | 2.42 | 14.71 | 2.51 | 1.59 |
BC2 | 9.72 | 13.18 | 1.56 | 13.18 | 1.56 | 14.06 | 1.91 | 1.22 |
Avg BC | 10.09 | 11.91 | 1.57 | 14.87 | 1.99 | 14.39 | 2.21 | 1.41 |
CSC1 | 21.45 | 14.40 | 0.66 | 30.12 | 3.10 | 29.90 | 3.89 | 5.92 |
CSC2 | 25.61 | 14.74 | 0.62 | 27.42 | 2.44 | 24.39 | 2.92 | 4.68 |
Avg CSC | 23.53 | 14.57 | 0.64 | 28.77 | 2.77 | 27.15 | 3.41 | 5.3 |
Improvement (%) | 133 | 22 | − 59 | 93 | 39 | 87 | 54 | 276 |