Skip to main content

Official Journal of the Japan Wood Research Society

Table 1 Specific data for mechanical properties and mechanical properties/density

From: Effect of temperature on color changes and mechanical properties of poplar/bismuth oxide wood alloy during warm-press forming

Temperature (℃) Density (g/cm3) MOR (MPa) MOR/ density MOE (MPa) MOE/ density HV (Kgf/mm2) HV/ density
100 1.86 39.72 21.35 5136 2761.29 13.63 7.33
120 1.88 48.95 26.04 6420 3414.89 20.78 11.05
140 1.86 54.71 29.41 6424 3453.76 20.83 11.20
160 1.85 52.75 28.51 6069 3280.54 18.62 10.06
180 1.73 16.27 9.40 1433 828.32 13.78 7.97
200 1.69 7.13 4.22 861 509.47 10.66 6.31