Skip to main content

Official Journal of the Japan Wood Research Society

Table 2 Mean statistics of specimens

From: Experimental study of compressive properties parallel to grain of glulam

Sample statistics

Maximum stress fc,0 [N/mm2]

 

2.5-1Ce

10-1Ce

20-1Ce

20-2Ce

2.5-1Cy

10-1Cy

20-1Cy

20-2Cy

Quantity

6

6

6

6

6

6

6

6

Mean

31

33

34

33

47

44

45

44

CV [%]

6

5

2

3

5

3

2

5

 

Longitudinal modulus of elasticity in full height E L,f [N/mm2]

 

Mean

4383

4432

5349

6649

6823

6284

8242

10,091

CV [%]

19

5

4

1

20

6

5

4

 

Longitudinal modulus of elasticity in middle zone E L,m [N/mm2]

 

Mean

7549

8807

14,318

9722

14,966

15,247

22,575

14,847

CV [%]

12

14

34

8

11

15

18

8

Sample statistics

Maximum stress fc,0 [N/mm2]

2.5-1Sp

10-1Sp

20-1Sp

20-05Sp

20-3Sp

20-3bSp

20-3bxSp

20-3sSp

Quantity

6

6

6

6

6

4

4

4

Mean

53

44

44

47

41

41

41

42

CV [%]

12

6

3

1

1

4

2

4

 

Longitudinal modulus of elasticity in full height E L,f [N/mm2]

Mean

5327

4920

2507

1601

5510

2558

2381

2670

CV [%]

9

11

3

7

4

3

6

2

 

Longitudinal modulus of elasticity in middle zone E L,m [N/mm2]

Mean

13,155

12,440

13,950

13,414

11,865

13,240

12,500

14,064

CV [%]

13

9

16

18

5

9

10

11

  1. CV coefficient of variation