Table 1 Fundamental properties of rubberwood-based plywood/OSB used for this experiment

From: Developing structural sandwich panels for energy-efficient wall applications using laminated oil palm wood and rubberwood-based plywood/oriented strand board

Properties

Face materials

Testing standard

Plywood

OSB

Density (kg/m3)

695 ± 45 (n = 40)

(DS = 50 × 50 × 8)

738 ± 61 (n = 40)

(DS = 50 × 50 × 9)

[20]

Swelling (%)

  

[21]

 Major direction

0.42 ± 0.29 (n = 10)

0.29 ± 0.31(n = 10)

 

 Minor direction

0.32 ± 0.28 (n = 10)

0.44 ± 0.31(n = 10)

 

 Thickness direction

1.30 ± 0.25 (n = 10)

(DS = 50 × 50 × 8)

15.39 ± 2.39 (n = 10)

(DS = 50 × 50 × 9)

 

Compression parallel to surface (along major direction) (MPa)

21.0 ± 5.6 (n = 30)

(DS = 25 × 32 × 8)

10.6 ± 3.2 (n = 30)

(DS = 25 × 36 × 9)

[22]