Table 3 Measurement of the oven-dry density and moisture content after uniaxial compression testing the specimens

From: Mechanical properties of laminated bamboo lumber N-finity according to ISO 23478-2022

Sample no.

Length (mm)

Width (mm)

Height/depth (mm)

Volume (mm3) × 1000

Mass (g)

MC%

Density (kg/cm3)

0 h

3 h

2 h

\(l\)

\(b\)

\({h}_{0}\)

\({V}_{0}\)

m0

mdry

mi

\(\rho\)

2a

38.89

36.56

73.64

1047.02

69.8

64.5

64.5

7.59

616.03

4a

38.64

36.63

73.47

1039.88

68.9

64.1

64.0

6.96

616.41

6a

38.33

36.56

73.96

1036.43

71.5

66.4

66.4

7.13

640.65

8a

38.91

36.58

72.77

1035.75

65.8

61.1

61.1

7.14

589.91

12a

37.27

36.58

74.30

1012.96

67.0

62.4

62.4

6.86

616.01

4b

37.56

36.55

74.42

1021.65

72.2

66.6

66.6

7.75

651.88

7b

37.29

36.52

74.29

1011.70

70.5

65.5

65.5

7.09

647.42

9b

37.29

36.52

74.29

1011.70

71.5

66.4

66.4

7.13

656.31

15b

37.43

36.59

74.16

1015.66

70.7

65.6

65.6

7.21

645.88

16b

37.39

36.45

73.00

994.89

71.5

66.5

66.5

7.01

668.41

2c

36.95

36.79

73.05

993.03

65.2

60.1

60.1

7.82

605.21

9c

37.05

37.87

73.11

1025.79

68.2

63.3

63.3

7.18

617.08

10c

37.08

37.02

72.28

992.18

65.5

60.8

60.8

7.17

612.78

11c

37.12

36.74

72.86

993.65

64.2

59.7

59.7

7.01

600.81

13c

37.26

35.80

72.87

972.01

62.4

58.0

58.0

7.05

596.70

Mean

       

7.20

625.43

STD

       

0.27

23.41

  1. Letters in the sample no. indicate the sample group a, b or c